Pyrophyllite Data

‘ALSIL’ & ‘CERAMIT’ MACHINABLE CERAMIC

Property

Units

State

Unfired

Good thermal shock properties

Ceramit 10

Fired 800-1000°C

Good thermal shock properties

Ceramit 14

Fired 1300°C

Excellent electrical properties

Density

g/cm3

2.4-2.55

Colour

Grey

Pink to Dark Brown

Hardness

Mohs

2.5

5

7

Porosity

%

1.8-2

2.66 ± 0.02

0.01-Nil

Softening Temperature

°C

1600°C

Max.Continuous Temp.

°C

1100°C

Coefficient of linear thermal Expansion

X 10-6

20 – 600°C

2.9-3.5

6-8

Thermal Conductivity

W/mK

1.5

1.9

Compressive strength

KN/cm²

10.3

15.16

Cross bending strength

1.13 -1.58

3.37

8.27

Tensile strength

1.03

2.34

3.44

Volume resistivity

20

300

500 MΩ/cm3

700

900

Same

As

Ceramit14

When

dry

1014

109

106

105

104

Dielectric Strength

Kv (Using a 5mm thick test piece)

24

Power Factor

@1mHz tand x 104

0.1 – 0.13

Permitivity

5.2

T E Value

°C

700

Loss Factor

1000K/Hz

0.05


Visa & Mastercard accepted

© 2024 Ceramic Substrates and Components Ltd
Lukely Works, Carisbrooke Road, Newport, Isle of Wight, United Kingdom, PO30 1DH
Tel: +44 (0)1983 528697 - Email: info@ceramic-substrates.co.uk
Company Registration No.934853